search  current discussion  categories  glazes - specific colors 

cranberry or blood red!

updated tue 9 dec 97

 

Norm on thu 4 dec 97

Hey Folks,

I am looking for a glaze batch that will produce a Cranberry or Blood
red at cone 6 oxidation. Any favorites??

Thanks, Norm

Andrew Lubow on fri 5 dec 97

Here is an Ox Blood Red that I've used in the past. Apply it HEAVILY for the
best results.

Gerstly Borate 54.88%
Talc 14.63%
Flint 30.49%
100%
+ Red Iron Oxide 21.95%


----------
From: Ceramic Arts Discussion List on behalf of Norm
Sent: Thursday, December 04, 1997 8:06 AM
To: Multiple recipients of list CLAYART
Subject: Cranberry or Blood red!

----------------------------Original message----------------------------
Hey Folks,

I am looking for a glaze batch that will produce a Cranberry or Blood
red at cone 6 oxidation. Any favorites??

Thanks, Norm

Talbott on fri 5 dec 97

In Oxidation?????... fat chance... Try reduction ^8 - ^10. Using a copper
red recipe. Want reds then fire using a fossil fuel... Marshall

>----------------------------Original message----------------------------
>Hey Folks,
>
>I am looking for a glaze batch that will produce a Cranberry or Blood
>red at cone 6 oxidation. Any favorites??
>
>Thanks, Norm

101 CLAYART MUGS
2ND ANNUAL CLAYARTERS' GALLERY - NAPLES, MAINE (Summer 1998)
E-MAIL ME FOR AN APPLICATION
http://fmc.utm.edu/~dmcbeth/cag/naples.htm

Celia & Marshall Talbott, Pottery By Celia, Route 114, P O Box 4116,
Naples, Maine 04055-4116,(207)693-6100 voice and fax,(call first)
Clayarters' Live Chat Room, Fri & Sat Nites at 10 PM EDT & Sun at 1 PM EDT
http://webchat12.wbs.net/webchat3.so?Room=PRIVATE_Clayarters
---------------------------------------------------------------------

bryan on mon 8 dec 97

Norm wrote:
>
> ----------------------------Original message----------------------------
> Hey Folks,
>
> I am looking for a glaze batch that will produce a Cranberry or Blood
> red at cone 6 oxidation. Any favorites??
>
> Thanks, Norm
Norm:

Try this one.

Red/Pink/Purple/Mauve ^6 (try at ^5)

Gerstley Borate 21
Neph. Sy. 16
Kaolin 11
Whiting 20
Silica 32
Tin 5
Chrome .15

Anne Stecker