Mike Gordon on wed 3 dec 08


Cleaning out the studio and I ran across these glazes ( from a Jr.
College ) using Albany clay and remember that someone was interested in
some recipes. These are for C/7 and I don't remember having used them,
or whether it was oxidation or reduction, so do a test first!! They
were fired in a gas kiln, though, so it could be neutral.
Remember....... Manganese Dioxide is poisonous. Use caution when
handling. Mike Gordon
Albany............90........ a stony mat
Wollastonite...10
2% Bentonite

------------------------------------
Albany..........90......... yellowstone
Cryolite........10
2% Bentonite

---------------------------------------
Albany...........77.........cordovan brown
Kaolin............8
Mang. Diox...15
-------------------------------------
Albany........................90 ............black
Potash feldspar..........10
Colbalt Ox..................1
Mang.Diox..................2
Green Chrome Ox......2
Red Iron Ox................2