Dave Finkelnburg on tue 18 aug 09


Roxanne,=3D0A=3DA0=3DA0=3DA0 Short answer.=3DA0 There's no zinc in your rec=
ipe.=3DA0 If=3D
there were, one of the ingredients would be zinc oxide.=3DA0 That's the on=
ly=3D
form of zinc usually available unless it's hidden in some frit.=3DA0 There=
's=3D
no zinc in 3124.=3D0A=3DA0=3DA0=3DA0 Another short answer.=3DA0 In my expe=
rience, st=3D
ains with cobalt or copper will look good in a high calcium glaze like this=
=3D
.=3DA0 So will black.=3DA0 Most stains, in fact, will work.=3DA0 =3D0A=3DA0=
=3DA0=3DA0 Goo=3D
d glazing!=3D0A=3DA0=3DA0=3DA0 =3DA0=3DA0=3DA0 Dave Finkelnburg=3D0A=3DA0=
=3DA0=3DA0 http://www.ma=3D
ttanddavesclays.com/=3D0A=3D0A=3D0A=3D0A=3D0A______________________________=
__=3D0AFrom:=3D
Roxanne Hunnicutt =3D0ATo: Clayart@LSV.CERAMICS.ORG=3D0A=
Sent=3D
: Monday, August 17, 2009 10:41:57 PM=3D0ASubject: Leach Satin Clear from L=
es=3D
lie Lee R/OX x2 x5 custer 25.0 50.0 125.0 whiting 25.0 50.0 125.0 silica 25=
=3D
.0 50.0 125.0 Kaolin 25.0 50.0 125.0 Frit 3124 15.0 30.0 75.0 115.0 230.0 5=
=3D
75.0 Boy oh boy do I have the glaze for you. This gives you the most LUSH=
=3D
=3D0A=3D0ALeach Satin Clear from Leslie Lee R/OX x2 x5 custer 25.0 50.0 125=
.0 w=3D
hiting=3D0A25.0 50.0 125.0 silica 25.0 50.0 125.0 Kaolin 25.0 50.0 125.0 Fr=
it=3D
3124 15.0=3D0A30.0 75.0 115.0 230.0 575.0 =3D0A=3D0A=3D0A