DJ Brewer on tue 22 sep 09


Next topic!
Whose got a good oil spot glaze recipe?

much love
DJ

Des & Jan Howard on wed 23 sep 09


DJ
Assuming it wasn't a rhetorical question.
Greg Daley 'Glazes and Glazing Techniques'
Oilspot
Cone 10 oxidation
potash feldspar 59.68
mudgee limestone 6.2
talc 3.3
silica 30.83
+ red iron oxide 9.78
Works well.

John Britt 'The Complete Guide
to High-Fire Glazes' has a stack.
Des


DJ Brewer wrote:
> Next topic!
> Whose got a good oil spot glaze recipe?

--
Des & Jan Howard
Lue Pottery
Lue NSW
Australia
2850

02 6373 6419
www.luepottery.hwy.com.au
-32.656072 149.840624

John Britt on wed 23 sep 09


DJ,

I put a bunch in my book or just Google it,

John Britt
www.johnbrittpottery.com

Lee Love on wed 23 sep 09


On Tue, Sep 22, 2009 at 10:34 PM, DJ Brewer wrote:
> Next topic!
> Whose got a good oil spot glaze recipe?

DJ, check out John Britt's High Fire Glazes. You can get the
recipes on Google Books (but I do recommend buying the book!):


http://books.google.com/books?id=3DJiLJPahXYWgC&dq=3Dhigh+fire+glazes+john=
+britt&printsec=3Dfrontcover&source=3Dbn&hl=3Den&ei=3DhzS6SuGoD82M8AbT6NyMC=
g&sa=3DX&oi=3Dbook_result&ct=3Dresult&resnum=3D4#v=3Donepage&q=3Doil%20spot=
&f=3Dfalse


--
--
Lee Love, Minneapolis
"The tea ceremony bowl is the ceramic equivalent of a sonnet: a
small-scale, seemingly constricted form that challenges the artist to
go beyond mere technical virtuosity and find an approach that both
satisfies and transcends the conventions." -- Rob Sliberman
full essay: http://togeika.multiply.com/journal/item/273/

Gower on thu 24 sep 09


Hi Des Do you have an oil spot pic on your website
Debby
Australia
----- Original Message -----
From: "Des & Jan Howard"
To:
Sent: Wednesday, September 23, 2009 11:07 PM
Subject: Re: oil spot glaze recipe


> DJ
> Assuming it wasn't a rhetorical question.
> Greg Daley 'Glazes and Glazing Techniques'
> Oilspot
> Cone 10 oxidation
> potash feldspar 59.68
> mudgee limestone 6.2
> talc 3.3
> silica 30.83
> + red iron oxide 9.78
> Works well.
>
> John Britt 'The Complete Guide
> to High-Fire Glazes' has a stack.
> Des
>
>
> DJ Brewer wrote:
>> Next topic!
>> Whose got a good oil spot glaze recipe?
>
> --
> Des & Jan Howard
> Lue Pottery
> Lue NSW
> Australia
> 2850
>
> 02 6373 6419
> www.luepottery.hwy.com.au
> -32.656072 149.840624
>