Bill Merrill on wed 25 nov 09


Tom Spleth has a hand building, throwing and casting body that fires
between cone 8 and 10 either in reduction or oxidation. A tough body,
holds shape in firing. Releases easily from mold. =3D20

This formula is in Val Cushings hand book on page 24. It is well
advised for potters at all levels to own this handbook. I look at it
and it nearly parallels my notes in Val's class. I still have my notes
after 36 years and the dates and time of each lecture on every page.
Those were great times .....

=3D20

This hand book will answer so many questions for potters...

=3D20

Val Cushing's Handbook ( $28.00 )
1497 Waterwells Rd.,

RR 1,Box 236,

Alfred Station' N.Y., 14803.

=3D20

=3D20

18 Custer Feldspar

30 Grolleg or English China clay

12 Velvacast

8 Ball clay

12 Flint

12 Pyrotrol (pyrax)

=3D20

Water 40%

Darvan 00.35 %