search  current discussion  categories  glazes - cone 8-10 

^9 blue matt glaze request

updated sat 20 dec 97

 

Tracy Wilson on thu 18 dec 97

Howdy Folks...
I've been working with a glaze for the past couple of years. Adjusting it =
this
way and that. It is unreliable to say the least. Bubbles and blisters on =
half
the pots and the other half are GORGEOUS. When it is good, it is very, very
good and when it is bad...
Does anyone have a glaze they are willing to share? =5E9, reduction, no =
barium,
looks kinda like an ash glaze, antique (slate) blue with almost a hint of
green, satin matt to matt surface... for me to test?
Thanks so much,
Tracy

=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F==
5F=5F=5F=5F
Tracy Wilson
Saltbox Pottery
=234 Shaw Rd.
Woolwich, ME 04579
phone: 207-443-5586
fax: 207-443-6544
email: saltbox=40ime.net
web: http://www.ime.net/=7Edwilson/
=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F==
5F=5F=5F=5F

Arturo M DeVitalis on fri 19 dec 97

chk the clayart glazebase for val cushing blue

LizzardOL on fri 19 dec 97

A glaze was posted on the list a while ago called Clemson Univ. Satin Blue
Green Matt. I've tested it and it might be what your looking for:


Blue green Satin Matt Clemson U

Custer Spar 38.5
Whiting 20
EPK 20
Flint 15
Cobalt Carbonate 1
Rutile 6

It is a matt light blue where thick and greenish where thin. Very nice.

Liz Dodge in Berkeley, CA

In a message dated 12/18/97 2:52:41 PM, you wrote:

<
I've been working with a glaze for the past couple of years. Adjusting it =

this

way and that. It is unreliable to say the least. Bubbles and blisters on =

half

the pots and the other half are GORGEOUS. When it is good, it is very, very

good and when it is bad...

Does anyone have a glaze they are willing to share? =5E9, reduction, no =

barium,

looks kinda like an ash glaze, antique (slate) blue with almost a hint of

green, satin matt to matt surface... for me to test?