Louis Katz on mon 9 aug 10


Albany Slip Glaze

Albany Slip 100

Edouard Bastarache on mon 9 aug 10


+3% Cobalt carbonatre for a black glaze.

Gis,

Edouard Bastarache
Spertesperantisto

Sorel-Tracy
Quebec

http://www.flickr.com/photos/30058682@N00/
http://edouardbastarache.blogspot.com/
http://blogsalbertbastarache.blogspot.com/
http://cerampeintures.blogspot.com/
http://perso.wanadoo.fr/smart2000/index.htm



----- Original Message -----
From: "Louis Katz"
To:
Sent: Monday, August 09, 2010 7:23 AM
Subject: Re: Albany slip glaze recipes


Albany Slip Glaze

Albany Slip 100