randy mccall's "moving day" recipe.

updated tue 10 aug 10

 

Lili Krakowski on mon 9 aug 10


I call this a "Moving Day" Recipe. Because on Moving Day (or night =3D
before) one takes everything out of the fridge and serves/ eats it. =3D
Some things can be combined, an omelet covers a multitude of "fridge =3D
orphans" etc.

Recipe Name: moving day

16.2 Spodumene--Gwalia
44.8 Feldspar--Custer
14.6 Dolomite
8.1 Bone Ash
13 Red Art
3.2 Bentonite

99.9 Total


Unity Oxide
.114 Li2O
.067 Na2O
.148 K2O
.229 MgO
.443 CaO
1.000 Total

.398 Al2O3
.02 Fe2O3

2.343 SiO2
.005 TiO2
.066 P2O5

5.9 Ratio
73.1 Exp

Calculations by GlazeMasterT

This is so close to original in actual ingredients you might well get =3D
something like this if you got a new supply of Spod,. or Custer, or Red =3D
Art.

I have been using Bentonite in my recipe calculations sometimes even =3D
using only B as clay... since Carol Marians sent me a recipe that did =3D
just that.

I did not add your colorants because they would affect nothing.
Lili Krakowski
Be of good courage