Lili Krakowski on tue 31 aug 10
When we were talking abut Crocus Martis a few weeks back, Deb Thurman =3D
wanted the recipe for the glaze using it, which I had talked about.
It took me a while to find the Lee Center folder...because it is at Lee =3D
Center that I used that glaze, got recipe.
It is a Randi Red--and I seem to remember it was attributed to Sarah =3D
Bodine.
Recipe Name: lee center randi red
Cone: Color: =3D20
Firing: Surface: =3D20
Amount Ingredient
30 Silica
5 Kaolin--EPK
14 Talc
20 Feldspar--Kona F4
32 Gerstley Borate--9/97
7.65 Crocus Martis
7.65 Fe2O3
Unity Oxide
.148 Na2O
.034 K2O
.413 MgO
.405 CaO
.193 Al2O3
.407 B2O3
.004 Fe2O3
2.941 SiO2
60.6 Exp
-----------------------------------
Calculations by GlazeMasterT
Note that the Alumina is a tidge low by Ron/John's standards as is COE .
Lili Krakowski
Be of good courage
| |
|