For those that are interested.
=3D20
Recipe Name: C HARRIS TEMMOKU
Cone: 6 Color: TEMMOKU
Firing: Oxidation Surface: Glossy
Amount Ingredient
18.6 Nepheline Syenite
8.5 Gerstley Borate--1999
9.3 Dolomite
9.3 Talc
18.6 Ball Clay Number 1
28.2 Silica
7.5 Bone Ash
100 Total
Additives
11 Iron Oxide--Red
Unity Oxide
.104 Na2O
.032 K2O
.359 MgO
.505 CaO
1.000 Total
.323 Al2O3
.094 B2O3
.005 Fe2O3
2.907 SiO2
.008 TiO2
.067 P2O5
9 Ratio
61 Exp
Comments: =3D20
-----------------------------------
Calculations by GlazeMaster=3D99
www.masteringglazes.com
------------------------------------
Randy