Karen Gringhuis on mon 11 oct 10


Cushing's HANDBOOK incl. a Jasper Ware recipe as ff:

C/9 vitreous shiny

C & C ball clay 30%
Cornwall Stone 60
Flint 10
total 100%
Macaloid 2%

Footnote: "Firing only to C/8 might be better"=3D20

He describes this as a totally vitreous almost self-glazing body. Adding=
=3D
2
- 4% Cobalt Oxide should give strong blue color. BLUNGE the macaloid in =
=3D
hot
water the night before mixing!!!

Eric Hansen on tue 12 oct 10


Karen: Interesting however that kind of Cornwall Stone is scarce;
maybe substitute a line blended % of new the new Cornwall Stone and
Fluorspar?
- h a n s e n

On Mon, Oct 11, 2010 at 4:05 PM, Karen Gringhuis wrot=
=3D
e:
> Cushing's HANDBOOK incl. a Jasper Ware recipe as ff:
>
> C/9 =3DA0vitreous shiny
>
> C & C ball clay =3DA0 =3DA0 =3DA0 30%
> Cornwall Stone =3DA0 =3DA0 =3DA0 60
> Flint =3DA0 =3DA0 =3DA0 =3DA0 =3DA0 =3DA0 =3DA0 =3DA0 =3DA0 =3DA0 =3DA010
> =3DA0 =3DA0 =3DA0 =3DA0total =3DA0 =3DA0 =3DA0 =3DA0 =3DA0 =3DA0 100%
> Macaloid =3DA0 =3DA0 =3DA0 =3DA0 =3DA0 =3DA0 =3DA0 =3DA0 =3DA0 2%
>
> Footnote: =3DA0"Firing only to C/8 might be better"
>
> He describes this as a totally vitreous almost self-glazing body. =3DA0Ad=
di=3D
ng 2
> - 4% Cobalt Oxide should give strong blue color. =3DA0BLUNGE the macaloid=
i=3D
n hot
> water the night before mixing!!!
>



--=3D20
Eric Alan Hansen
Stonehouse Studio Pottery
Alexandria, Virginia
americanpotter.blogspot.com
thesuddenschool.blogspot.com
hansencookbook.blogspot.com
"To me, human life in all its forms, individual and aggregate, is a
perpetual wonder: the flora of the earth and sea is full of beauty and
of mystery which seeks science to understand; the fauna of land and
ocean is not less wonderful; the world which holds them both, and the
great universe that folds it in on everyside, are still more
wonderful, complex, and attractive to the contemplating mind." -
Theodore Parker, minister, transcendentalist, abolitionist (1810-1860)

Karen Gringhuis on wed 13 oct 10


Eric -=3D20

"Fluorspar" =3D3D CaF4 i.e. NOT a good idea. My understanding is that it
volatilizes and can cause bloating and other problems. There are other
sources of calcium.=3D20

KG

Edouard Bastarache on wed 13 oct 10


Eric,

this one was published in Ceramics Monthly years ago :

C/6



LEPIDOLITE

62.50 %





FLUORSPAR

35.00 %



97.50 %




Gis,

Edouard Bastarache
Spertesperantisto

Sorel-Tracy
Quebec

http://www.flickr.com/photos/30058682@N00/
http://edouardbastarache.blogspot.com/
http://blogsalbertbastarache.blogspot.com/
http://cerampeintures.blogspot.com/
http://www.facebook.com/edouard.bastarache



----- Original Message -----
From: "Karen Gringhuis"
To:
Sent: Wednesday, October 13, 2010 12:41 PM
Subject: Re: JASPER WARE RECIPE


Eric -

"Fluorspar" =3D CaF4 i.e. NOT a good idea. My understanding is that it
volatilizes and can cause bloating and other problems. There are other
sources of calcium.

KG