search  current discussion  categories  glazes - cone 4-7 

cone 6 iron red glaze

updated thu 28 oct 10

 

Heather Bessey on wed 27 oct 10


From a long time lurker. Thank you all clayarters. You have provided much=
=3D
needed help and entertainment.
Mastering Cone 6 Glazes by Ron and John has allowed me to make functional p=
=3D
ottery and feel safe.
I have been using an iron red glaze for non food surfaces and now want to u=
=3D
se it on plates. I am willing to=3D20
change to another. I have used Randy's Red or Bob's Deep River Red. In qu=
=3D
estion are:
=3D20
Bob's Deep River Red Randy's Red
=3D20
flint 27.27 flint =
=3D
30
EPK 18.18 EPK =
=3D
5
neph sy 18.18 G-200 =
=3D
20
bone ash 9.09 talc =
=3D
15=3D20
dolomite 9.09 gerstly bora=
=3D
te 30
gerstly borate 9.09
talc 9.09
=3D20
red iron oxide 15 red iron oxi=
=3D
de 15 =3D20
=3D20
Thank you
Heather =3D