Judy on tue 2 nov 10
Randy, Thanks for posting the recipe for this green glaze. Question: =3D
What is Ball Clay #1? Tennessee? Kentucky? Doesn't matter? Thanks.
Judy Musicant
PottersGuildNJ.org
Cone: 6 Color: GREEN
Firing: Oxidation Surface: Glossy
Amount Ingredient
44.2 Nepheline Syenite
25.2 Gerstley Borate--1999
18.9 Silica
11.7 Ball Clay Number 1
100 Total
Additives
3 Copper Carbonate
4 Rutile
5 Tin Oxide
Comments: Adjusted from Chappell's Floating Blue. Gives a nice warm jade =
=3D
green glaze. Three thick coats brushed.
Great green glaze. 4% copper carbonate will give an iridescent green. 2% =
=3D
copper carbonate will give a celadon light green.
| |
|