search  current discussion  categories  glazes - traditional iron glazes 

shino disaster..problem found!

updated fri 12 nov 10

 

Gwynneth Rixon on thu 11 nov 10


Hi all- many thanks for the suggestions. The problem? Working in a small
space=3D2C overtired and needing to do the job yesterday I mixed in China=
=3D20
Clay (Kl on the tub) as I followed the wrong recipe. It should have=3D20
been Potash Feldspar!! (KF)

The good news is that I now know that I have a tub of orange slip-which exp=
=3D
lains the crawling!!

Back to mix the right ingredients when it gets light tomorrow morning.

Much blushing!!!

Thanks again!!

Gwynneth