Recipe Name: C HARRIS TEMMOKU
Cone: 6 Color: Iron Red
Firing: Oxidation Surface: Glossy
Amount Ingredient
18.6 Nepheline Syenite
8.5 Gerstley Borate--1999
9.3 Dolomite
9.3 Talc
18.6 Ball Clay Number 1
28.2 Silica
7.5 Bone Ash
100 Total
Additives
11 Iron Oxide--Red
Randy