Here are some low fire satin glaze recipes I have used:
they will be more satin/matt at 06 and more glossy at 04

Recipe Name: Hersch Emerald Green

Cone: 06-04 Color: emerald green
Firing: Oxidation Surface: Semiglossy

Amount Ingredient
31.5 Gerstley Borate--9/97

8.7 Nepheline Syenite
4.2 Kaolin--EPK
34.9 Silica
16.6 Whiting

95.9 Total

Additives
8 Copper Carbonate

Unity Oxide
.112 Na2O
.015 K2O
.085 MgO
.788 CaO
1.000 Total

.118 Al2O3
.381 B2O3
.003 Fe2O3

2.233 SiO2
0 TiO2
0 P2O5

19 Ratio
7 Exp

Comments: NOT FOR FOOD SURFACES. This is a glaze recipe I got from Sandi
Pierantozzi.
This glaze CANNOT BE REFIRED.
Calculations by GlazeMaster=3D99
www.masteringglazes.com
------------------------------------
Recipe Name: Hersch Gold/Ochre

Cone: 05 Color: gold/ochre
Firing: Oxidation Surface: Semimatte

Amount Ingredient
31.5 Gerstley Borate--9/97
8.7 Nepheline Syenite
8.7 Lithium Carbonate
4.2 Kaolin--EPK
34.9 Flint
16.6 Whiting

104.6 Total

Additives
8 Iron Oxide--Yellow

Unity Oxide
.247 Li2O
.08 Na2O
.01 K2O
.061 MgO
.602 CaO
1.000 Total

.083 Al2O3
.272 B2O3
.002 Fe2O3

1.522 SiO2
0 TiO2
0 P2O5

18.3 Ratio
7.2 Exp

Comments: this is Hersch glaze with yellow iron oxide, and lithium. It can
be refired. NOT FOR FOOD SURFACES. You can also try adding 1-2% cobalt carb
for blue instead of the copper or YIO.
-----------------------------------
Calculations by GlazeMaster=3D99
www.masteringglazes.com
------------------------------------


--=3D20
Sharon La Rocca Miranda
www.sharonmiranda.com