John Britt on wed 24 aug 11
n Diego NCECA?
Roxqnne,
Could be:
GOLDEN FAKE ASH Cone 6=3D20
28.0 Redart
24.5 Dolomite
21.0 Ball Clay
10.0 Gerstley Borate
9.5 Strontium Carbonate=3D20
5.0 Bone Ash
2.0 Lithium Carbonate
Here is a link:=3D20=3D20
http://ncclayclub.blogspot.com/2008/09/golden-fake-ash-cone-6.html
or=3D20
Matt Cone 6 reduction=3D20
Neph Sy..............55=3D20
Dolomite............. 11.5=3D20
Strontium Carb... 11.5=3D20
OM4 Ball Clay.... 7=3D20
Flint.................. 3=3D20
Gerstley Borate... 9=3D20
Add iron to taste,
Johnbrittpottery.com
Steve Slatin on wed 24 aug 11
n Diego NCECA?
Sounds a little like Diana Pancioli's fake ash glaze. IIRC, it's
in the archives.
Steve Slatin --=3D20
N48.0886450
W123.1420482
--- On Wed, 8/24/11, Roxanne Hunnicutt wrote:
> Do any of you have a memory of a flux
> rich strontium matte that had a
> beautiful iron response? The glaze came to us as a shared
> glaze=3DA0 group
> during the San Diego NCECA. A woman passed out glaze
> samples of cone 6
> reduction glazes and it was included among them.=3DA0 It
> used strontium Carb.
> rather than calcium or barium for the effect. (It is not
> the Pinell matte.)
> It runs in rivulets like a wood ash "irabo" type glaze. It
> is not the Pinell
> matte.
> *
> *
>
| |
|