Here's one I have in my records:
Voulkos Clay body
25 Goldart
25 Coarse Fireclay
25 OM4 Ball
12.5 Custer
12.5 EPK
3.75 Coarse Grog
Warm regards,
June
http://wwww.shambhalapottery.blogspot.com
http://groups.yahoo.com/group/sodasaltfiring/
http://www.shambhalapottery.com
----- Original Message -----
From: Donn Buchfinck
To: Clayart@LSV.CERAMICS.ORG
Sent: Sun, 11 Sep 2011 18:04:17 -0000 (UTC)
Subject: Pete Voulkos clay?
Does anyone have the clay recipe for the clay Pete used?
Please email me off list at donnbuchfinck@gmail.com
Thank you,
Donn Buchfinck
www.donnbuchfinck.com
www.youtube.com/bayareaartist999
James A. Monk on mon 12 sep 11
Donn,
I found the message below at http://www.potters.org/subject09589.htm
James A. Monk
---------------------------------------------------------------------------=
-
------
Brandon Phillips on Monday 1 February 10
Craig-
I have this in a notebook, I can't remember the source though but I seem to
remember it being legitimate...who knows though.
Voulkos Clay
100 Goldart
100 Coarse Fireclay
100 OM4 Ball
50 Custer
50 EPK
15 Coarse Grog
Brandon Phillips
www.supportyourlocalpotter.com
-----Original Message-----
From: Clayart [mailto:Clayart@LSV.CERAMICS.ORG] On Behalf Of Donn Buchfinck
Sent: Sunday, September 11, 2011 1:04 PM
To: Clayart@LSV.CERAMICS.ORG
Subject: Pete Voulkos clay?
Does anyone have the clay recipe for the clay Pete used?
Please email me off list at donnbuchfinck@gmail.com
Thank you,
Donn Buchfinck
www.donnbuchfinck.com
www.youtube.com/bayareaartist999
| |
|