charcoal glaze, what cone?

updated fri 2 dec 11

 

Amy Romaniec on thu 1 dec 11


interested but what ^ is this glaze?

> Date: Thu=3D2C 1 Dec 2011 22:51:52 +0800
> From: ricswenson0823@HOTMAIL.COM
> Subject: Re: Charcoal glaze
> To: Clayart@LSV.CERAMICS.ORG
>=3D20
> potssh feldspar 38.05
> flint 9.91
> Kaolin EPK 20.17
> whiting 16.19
> zinc oxide 4.15
> rutile 2.65
> tin oxide 1.76
> nickel oxide 3.50
> iron oxide red 3.50
>=3D20
>=3D20
> black or charcoal..color.
>=3D20
> try it.
>=3D20
> ric
>=3D20
> Ric Swenson=3D2C B.F.A=3D2C M.F.A.
> Ceramist=3D2C Artist and Teacher.
> Jing De Zhen Ceramic Institute
> Jing De Zhen City=3D2C
> Jiang Xi Province
> China
> Mobile: 86-13767818872
>=3D20
>=3D20
>=3D20
> > Date: Thu=3D2C 1 Dec 2011 06:13:42 -0800
> > From: jetalbot@BELLSOUTH.NET
> > Subject: Charcoal glaze
> > To: Clayart@LSV.CERAMICS.ORG
> >
> > Does anyone know where I can find a picture of something glazed with "c=
=3D
harcoal
> > satin matt glaze"? Elaine
=3D