search  current discussion  categories  glazes - specific colors 

rutilr blue

updated sun 8 feb 98

 

Mike Speed on thu 5 feb 98

I am looking for the Rutile Blue ^10 formula that
appeared in CM in the 1980's

Thanks

Mike


___________________________________________________
F. Michael Speed
Department of Statistics
Texas A&M University
College Station, Tx 77843-3143
409-845-3182
409-845-3144 (Fax)

Jan Wax on sat 7 feb 98

>----------------------------Original message----------------------------
>I am looking for the Rutile Blue ^10 formula that
>appeared in CM in the 1980's
>
>Thanks
>
>Mike
>___________________________________________________
>F. Michael Speed
>Department of Statistics
>Texas A&M University
>College Station, Tx 77843-3143
>409-845-3182
>409-845-3144 (Fax)
Dear Mike,
I can't put my hands on that copy of CM right now, but I did copy into
my glaze notebook the two rutile glazes in that article. Rutile Blue II is
a glaze I am still using. Here they are:

Rutile Blue I
cone 11 Reduction
Custer Spar 28.9
Whiting 20.6
EPK 18.9
Flint 31.6
Rutile 7.0

Rutile Blue II
cone 10 Reduction
Dolomite 15.8
Custer Spar 30.0
Whiting 11.1
EPK 16.8
Flint 26.3
Rutile 8.0