search  current discussion  categories  glazes - cone 8-10 

crystalline glazes (cone 8)

updated thu 19 feb 98

 

The Allens on tue 17 feb 98

Marc,
Check out Lasse Ostman's web site.....lots of beautiful crystalline glaze
formulas (which I hope to try out one of these days....) Cone 8-9.
Carla Allen
ridgerun=40scrtc.blue.net

Dave Eickholt on wed 18 feb 98

Try Aaonsen & Johnson Crystalline Glaze

Ferro Frit 3110 65 pbw
Zinc oxide 25
Silica 15
total 100 grams
Plus 2%
titianium dioxide
will yield white

add other oxides also with titianium ex
2% copper carb. & 1/2 % cobalt carb .
will give a blue crystal /green background
holding temp.after melt cone 8 should be about 1900 to 1850 F.