search  current discussion  categories  glazes - specific colors 

reeves green

updated sat 12 aug 00

 

Malone & Dean McRaine on sun 8 mar 98

Aloha all;
Anybody have a recipe for 'Reeve's Green'? It's a ^10 chrome green mainly
used for brush and trained decoration.

Dean from sunny Kauai

GURUSHAKTI@AOL.COM on thu 10 aug 00


Reeves Green Cone 10

Custer feldspar 75
whiting 15
EPK 5
Silica 5
Add:
Rutile 8%, Cobalt oxide 2%, Bentonite 2%