jetharrs@pacific.telebyte.net on wed 11 mar 98

So any of you have a glaze recipe for a warm grey glossy matt or shiny
glaze at cone 10 reduction?

--Asking for a friend

Thanks much,
Jeanette harris

Dan Wilson on thu 12 mar 98


I like this glaze. Don't know where it came from. My appologies to the
originator.

Grey Blue Celadon cone 8-10

Pspar 77.4
Flint 13.9
Whiting 5.9
Iron Ox. 2.2
Tin Ox. .6

Give it a try...

dan Wilson







>----------------------------Original message----------------------------
>So any of you have a glaze recipe for a warm grey glossy matt or shiny
>glaze at cone 10 reduction?
>
>--Asking for a friend
>
>Thanks much,
>Jeanette harris

B A HARPER on wed 18 mar 98

Hi Jeanette -
I was testing many different combinations of materials in a glaze and
ran across this very nice grey glaze :

Kaolin - 20
Custer spar - 50
Dolomite - 10
Whiting - 10
Flint - 10

It's a very simple glaze, but I got a real nice satiny grey that fit
perfectly and did not run even where thick. In my tests I always
referred to it as E#3. I was using a white stoneware throwing body
and fired it in an updraft cone 10 reduction, with a strong body
reduction at 06 and a light/moderate reduction from 06 to 10. Hope
this helps. E-mail me privately at DSWN57C@PRODIGY.COM and tell me
what you get.

- Brian Harper

Ron Roy on thu 19 mar 98

This looks like a durable glaze - it will probably craze on most porcelains
though.


>----------------------------Original message----------------------------
>Hi Jeanette -
>I was testing many different combinations of materials in a glaze and
>ran across this very nice grey glaze :
>
>Kaolin - 20
>Custer spar - 50
>Dolomite - 10
>Whiting - 10
>Flint - 10
>
>It's a very simple glaze, but I got a real nice satiny grey that fit
>perfectly and did not run even where thick. In my tests I always
>referred to it as E#3. I was using a white stoneware throwing body
>and fired it in an updraft cone 10 reduction, with a strong body
>reduction at 06 and a light/moderate reduction from 06 to 10. Hope
>this helps. E-mail me privately at DSWN57C@PRODIGY.COM and tell me
>what you get.
>
>- Brian Harper

Ron Roy
93 Pegasus trail
Scarborough Otario
Canada M1G 3N8
Phone: 416-439-2621
Fax: 416-438-7849
Web page: Home page http://digitalfire.com/education/people/ronroy.htm