cone 06-05 blue recipe request...

updated fri 24 apr 98

 

C Redding on mon 20 apr 98


Hi Clayarters! Just a quickie for you electric people out there: I need
a blue (any blu) cone 06-05 earthenware glaze recipe that is lead free,
safe to eat off of, dishwaher safe. Any good glazes out there that anyone
would be willing to share with me?

Thanks so much!!!


cookie

cr7696@ark.ship.edu

Jennifer Rhinesmith on wed 22 apr 98

Her's an ^04 Base and additions that may help. Hope you like it, I have
never tried it.

Frit 3124 40%
Gerstley Borate 30
Flint 5
Neph Sy 25
Zircopax 8

Additions:

White no additions
Yellow 3% Red Iron Oxide
Turquoise 2% Copper Carb.
Sky Blue 1% Cobalt Carb.
Purpleish Brown 2%Magnesium Dioxide
Green 2%Chrome Oxide
Salmon Pink 4%Mason 6006 Deep
Crimson Stain


>From owner-clayart@lsv.uky.edu Mon Apr 20 05:46:54 1998
>Received: from lsv (128.163.1.15) by lsv.uky.edu (LSMTP for Windows NT
v1.0a) with SMTP id D5755700 ; Mon, 20 Apr 1998 8:39:38 -0400
>Received: from LSV.UKY.EDU by LSV.UKY.EDU (LISTSERV-TCP/IP release
1.8b) with
> spool id 115162952 for CLAYART@LSV.UKY.EDU; Mon, 20 Apr 1998
08:37:14
> -0400
>Received: from UKCC.uky.edu by lsv.uky.edu (LSMTP for Windows NT v1.0a)
with
> SMTP id 7FE902A0 ; Mon, 20 Apr 1998 8:37:06 -0400
>Received: from UKCC.UKY.EDU by UKCC.uky.edu (IBM VM SMTP V2R3) with
BSMTP id
> 4748; Mon, 20 Apr 98 08:37:09 EDT
>Received: from ukcc.uky.edu (NJE origin LSTOWNR@UKCC) by UKCC.UKY.EDU
(LMail
> V1.2a/1.8a) with BSMTP id 8666; Mon, 20 Apr 1998 08:37:08
-0400
>Resent-Subject: Cone 06-05 blue recipe request...
>Received: from UKCC (NJE origin SMTP2@UKCC) by UKCC.UKY.EDU (LMail
V1.2a/1.8a)
> with BSMTP id 0180; Sun, 19 Apr 1998 12:20:47 -0400
>Received: from lsv.uky.edu (128.163.1.15) by UKCC.uky.edu (IBM VM SMTP
V2R3)
> with TCP; Sun, 19 Apr 98 12:20:44 EDT
>Received: from lsv (128.163.1.15) by lsv.uky.edu (LSMTP for Windows NT
v1.0a)
> with SMTP id 34254360 ; 19 Apr 1998 12:18:04 -0400
>Received: from ark.ship.edu by lsv.uky.edu (LSMTP for Windows NT v1.0a)
with
> SMTP id 33C37450 ; 19 Apr 1998 12:18:03 -0400
>Received: from localhost (cr7696@localhost) by ark.ship.edu
(8.8.6/8.8.6) with
> SMTP id MAA14905 for ; Sun, 19 Apr 1998
12:19:40
> -0400 (EDT)
>MIME-Version: 1.0
>Content-Type: TEXT/PLAIN; charset=US-ASCII
>X-Mailer: MailBook 96.02.327
>MIME-Version: 1.0
>Content-Type: TEXT/PLAIN; charset=US-ASCII
>Content-Transfer-Encoding: 7BIT
>Approved-By: List Moderator
>Message-ID:
>Date: Mon, 20 Apr 1998 08:37:05 EDT
>Reply-To: Ceramic Arts Discussion List
>Sender: Ceramic Arts Discussion List
>From: C Redding
>Subject: Cone 06-05 blue recipe request...
>To: Multiple recipients of list CLAYART
>
>----------------------------Original
message----------------------------
>
>Hi Clayarters! Just a quickie for you electric people out there: I
need
>a blue (any blu) cone 06-05 earthenware glaze recipe that is lead free,
>safe to eat off of, dishwaher safe. Any good glazes out there that
anyone
>would be willing to share with me?
>
>Thanks so much!!!
>
>
>cookie
>
>cr7696@ark.ship.edu
>
>


********************************
Jennifer Rhinesmith
P.O. Box 995
Alpine, Tx 79831
jrpots@hotmail.com


______________________________________________________
Get Your Private, Free Email at http://www.hotmail.com

Cheryl Fisher on thu 23 apr 98

The following is from a Woody Hughes workshop I took at Arrowmont last
summer. They've all been published in Ceramics Monthly.

Woody's Base c04
Gerstley Borate 26
Neph Sy 20
3124 30
Lithium Carbonate 4
EPK 10
Flint 10

Light Green add 2% copper carb.
Dark Green add 6% copper carbonate
Dark Blue add .5% cobalt
Yellow add 4% red iron oxide

He was brushing his glazes, using with and over terra sig and colored
slips.

Cheryl
Sarasota, FL