Susan,
Here are a few Barium Matt Glazes I have tried. Please take care when
handling Barium.
- Gary Wang
Barium Blue Matt from Vivika and Otto Heino Cone 5-10
Barium Carbonate 60
Nepheline Syenite 130
Kentucky Ball Clay 14
Flint 16
Lithium Carbonate 6
Copper Carbonate 6
Fairbanks Blue Cone 8-9-10 from GlazeBase at SDSU
Barium Carbonate 30
Custer Spar 60
Nepheline Syenite 5
EPK 5
Copper Carbonate 6
Bentonite 1
Dean Blue Cone 8-9-10 from GlazeBase at SDSU
Custer Spar 65
Barium Carbonate 35
Copper Oxide 4.35
Bentonite 3
| |
|