Fabienne on sun 26 jul 98
Hello,
I am developing my first glaze, be gentle with me, tear the glaze apart
anyway you want :) I am using Insight to calculate it. Any comments about
potential problems or ways to make it better, etc. are more than welcome.
Thank you
FM072698 - ^6 Clear Base for Tucker's MCS
=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=
=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D=3D
WOLLASTONITE........ 3.50 3.50%
EPK KAOLIN.......... 21.75 21.75%
FRIT 3134........... 36.75 36.75%
SILICA.............. 24.50 24.50%
G-200 FELDSPAR G200. 9.00 9.00%
=3DSTRONTIUM CARBONATE. 4.50 4.50%
=3D=3D=3D=3D=3D=3D=3D=3D
100.00
CaO 0.60* 9.58%
MgO 0.00* 0.04%
K2O 0.04* 1.09%
Na2O 0.24* 4.26%
SrO 0.11* 3.30%
TiO2 0.00 0.09%
Al2O3 0.36 10.38%
B2O3 0.45 8.88%
P2O5 0.00 0.05%
SiO2 3.64 62.12%
Fe2O3 0.00 0.21%
MnO 0.00* 0.00%
Cost/kg 1.91
Si:Al 10.16
SiB:Al 11.42
Expan 7.00
=A4=BA=B0`=B0=BA=A4=F8,=B8=B8,=F8=A4=BA=B0`=B0=BA=A4=F8,=B8=B8,=F8=A4=BA=B0`=
=B0=BA=A4=F8,=B8=B8,=F8=A4=BA=B0`=B0=BA=A4=F8,=B8=B8,=F8=A4=BA=B0`
Fabienne | Yes, I have learned from my
http://www.vivelafrance.org | mistakes... =20
| I can reproduce them exactly.
| |
|