Marcia Selsor on sun 8 nov 98
reposting this base from last week.
Here is a nice base glaze we use for ^6 reduction.We call it White Liner.
> > been using it so long I don't remember the source.
> >
> > Ger. Bor. 20
> > Neph Sy 30
> > EPK 13.3
> > Whiting 9.4
> > Talc 17.2
> > Flint 10
> >
> > Zircopax 15
> >
> > for other colors add:
> > 3% iron Oxide
> > 5% rutile = Pumpkin/or Oakleaf
> >
> > 3% iron
> > 3% rutile = spicy mustard
> >
> > .5 cobalt carb
> > .5 rutile = light blue
> >
> > 3% rutile= gold
> >
| |
|