search  current discussion  categories  techniques - stains 

1952 underglaze/ stain recipes, continued

updated thu 3 dec 98

 

Reid Harvey on wed 2 dec 98

from: Reid Harvey
Ceramiques d'Afrique d'Abidjan
la Cote d'Ivoire

As promised here is the continuation of underglaze/ stain recipes from
the January 1952 issue of Ceramic Industry (excluding those with lead):

VICTORIA GREEN
36% Potassium Dichromate
20 Flint
18 Fluorospar
26 Whiting

CRIMSON
20.8% Flint
22.9 Whiting
6.6 Calcium Sulphate
4.4 Fluorospar
43.7 Tin Oxide
1.6 Potassium Dichromate

TURQUOISE
18.2% Copper Sulfate, Calcined
36.4 Slaked Lime
36.4 Flint
9.0 Sodium Chloride

BLUE GREEN
41.8% Cobalt Oxide
19.2 Chrome Oxide
39.0 Aluminum Oxide

PEA GREEN
36% Potassium Dichromate
12 Fused Calcium Chloride
20 Flint
20 Whiting
12 Fluorospar

DARK GREEN
20% Potash Feldspar
10 China Clay
20 Flint
25 Potassium Dichromate
25 Chrome Oxide

OLIVE GREEN
37% Flint
15 Zinc Oxide
18 Borax
22 Chrome Oxide
8 Cobalt Oxide

LIGHT BLUE
25% Cobalt Oxide
25 Zinc Oxide
50 Alumina

VIOLET BLUE
15% Cobalt Oxide
28 Magnesia
57 Alumina

BLACK
43% Iron Oxide
43 Chrome Oxide
10 Manganese Dioxide
4 Cobalt Oxide

DARK PINK
19.0% Flint
17.1 Whiting
47.6 Tin Oxide
7.6 Fluorospar
4.8 Selenium
2.9 Potassium Dichromate
1.0 Iron Chromate

END