Cone 10 reduction

Nepheline syenite....36.8
dolomite....11.9
whiting....8.0
barium carbonate....6.4
kaolin....2.1
flint....34.8
red iron oxide....2
rutile...5

This is another rutile blue glaze that is dark blue where thick
and orange where thin.
I haven't used it since the '70's, and stopped using it because
it looks virtually the same as "#51 Rutile Blue", a glaze I sent to
Clayart a few weeks ago (See below).
#51 is cheaper and avoids the hazards of handling barium
carbonate.
Xavier, I hope you get some 'extra credit' from your teacher for
finding the glaze.

David Hendley
Maydelle, Texas


#51 Rutile Blue, from Big Creek Pottery, Davenport, California, 1973

Feldspar (I've used all kinds, they all worked).....357
Flint.....436
Whiting.....159
Kaolin.....137
Red Iron Oxide.....50
Rutile.....50



At 01:33 PM 10/20/98 EDT, you wrote:
>----------------------------Original message----------------------------
>Hi Everyone!!
>I'm desperately seeking a glaze for my teacher. Its a cone 10 reduction
glaze
>called "Orange Blue Breakfast Special" it is from Claremont collage in
>California. If anyone can help me I would really appreciate it.
>
>thanks,
>Xavier
>