search  current discussion  categories  glazes - traditional iron glazes 

celedon recipie

updated sat 31 oct 98

 

Donn Buchfinck on fri 30 oct 98

1234 celedon c10

kaolin 10
whiting 20
custer spar 40
flint 30

tin ox 1%
barnard slip clay 7%

barnard slip clay is called blackbird sometimes
if the glaze crazes real bad, do a line blend adjusting the silica content
and this will help the glaze to fit
if you want a nice chun blue use grolleg kaolin
if you want a green use 6 tile kaolin

V.C. Lung Chuan c10

Custer spar 30
whiting 19
flint 30
epk 8
barnard slip clay 4
wood ash 6
ball clay 3


red iron ox 1%