search  current discussion  categories  people 

lana wilson's chrome red

updated wed 13 jan 99

 

Ann Stecker on tue 12 jan 99

Here is the Chrome Red glaze from Lana Wilson's book. Several people
have contacted me asking for it so I thought there may be others
interested. I've posted this before and forgot the decimal point in
front of the 15!!!! Many noticed.

Chrome Red ^6

Gerstley Borate 21
Neph Sy 16
Kaolin 11
Whiting 20
Silica 32
Tin 5
Chrome .15

Good Luck!

Anne Stecker
rekcets@open.org