search  current discussion  categories  kilns & firing - raku 

my raku glazes..

updated thu 10 dec 98

 

ababy sharon on wed 9 dec 98

Or should I say :The glazes I use:My Main Frit =3BVO6004p of =
Reimbold=26Srick
NaO:11.5
K2O:15.5
AL2O3:3.5
Si2O3:44
=
B2O3=3B25.5

Base:AA Clear, White:
Frit=3B6004: 80
Whiting: 15
BallClay 8
Bentonite 2

AA-2,Green:Add-1chrome Ox.
1 Copper Car.


AA3Blue(Not for reduction):
Add:-3 Copper Ox.


AA-5 Dark Green:Add=3B-1.5 Cobalt Ox.
2 Chrome Ox.


AA -7 Olive Green:Add -6 copper Ox.


AA-11.Here I tryed to get a softer blue :

So,add: 0.25 Cobalt Ox.
0.25 Red Iron ox.

10: Ziropax
1: Copper Ox.
15: Frit A2120p
(Another frit from the same manufacturer) :Na2O3: 27.6
Cao :6.2
Ai2O3:2.8-
SiO2: 63.4


Last Friday I tried a differt way:
AA11-2


Frit 3110: 80
Ziropax: 10
Bentonit: 5
Copper Ox:1
Cobalt car.:1
Ocher-Iron:3

Since being connected to the internet I got many ideas for shape and =
glaze=3BI
hope I can help you too.

Ababi.