search  current discussion  categories  glazes - cone 8-10 

cone 9 rutile glaze

updated mon 1 mar 99

 

Flat Earth Clay Works, Inc. on sat 27 feb 99

We are looking for a cone 9 rutile glaze formula. If anybody out there has
had any experience with this we would appreciate any information that you
could pass along.
Thanks

Mike Schlyer

June Perry on sun 28 feb 99

Here's a cone 9 rutile blue I used to use in the 70's. It's best at cone 9
starting or around 2 or 3 o'clock, if memory serves me!

#166 WOO BLUE BROWN CONE 9 REDUCTION

WHITING 18
CUSTER FELDSPAR 42
BALL CLAY 13
FLINT 27
ADD: RED IRON OXIDE 4%, RUTILE 4%,BENTONITE 1%

Regards,