Maureen Collins on wed 10 mar 99
Does anyone have glaze recipes and firing info/stories for using the Naked
Raku and Candy Raku Glazes?
Thanks,
Maureen
Karen Shapiro on thu 11 mar 99
Hi Maureen,
Here's "Candy Luster Glaze" ^06
Gerstley Borate 70
Cornwall Stone 30
Tin Oxide
Karen Shapiro on thu 11 mar 99
Oops, sorry; this got sent unfinished!
Candy Luster Glaze
GB 70
Cornwall Stone 30
Tin Oxide 0.5
Cobalt Carb 0.25
Copper Carb 1.5
I have tested this glaze and got a beautiful blue with pink highlights,
pulling fast. The Cornwall gives a beautiful satiny sheen.
I don't know about the "naked raku".
Karen in Sonoma
| |
|