search  current discussion  categories  glazes - cone 8-10 

here's cone 10 waxy matt base for lavendar

updated sun 25 apr 99

 

June Perry on sat 24 apr 99

Cone 9-10 REDUCTION WHITE WAXY MATT
OPAQUE

CUSTER FELDSPAR 41
GERSLEY BORATE 12
DOLOMITE 7
TALC 15
KAOLIN 5
FLINT 20


FOR LAVENDAR 1/2% COBALT CARBONATE. If you want it to be more of a deep
purple add 1 to 1 1/2% cobalt carb. This is very bright lavendar!
Substituting Nepheline Syenite for the Custer may bring it down to cone 6.