isak on tue 27 apr 99
------------------
-----Ursprungligt meddelande-----
Fr=E5n: William Hewlett =3C105335.63=40compuserve.com=3E
Till: CLAYART=40LSV.UKY.EDU =3CCLAYART=40LSV.UKY.EDU=3E
Datum: den 26 april 1999 21:08
=C4mne: CRYSTALINE HALOS
----------------------------Original message----------------------------
------------------
Hallo over there.
Spring in Sweden and halos in the sky.
Halos in a crystalglaze:
You can produce halos from the inside of the crystal and out, and vice
verce.
Let=60s say that the topp-temp for a glaze is +1280C, take it down to =
+1180C,
stay for 15 minutes and then increase the temp +30 degrees C and down to
+1180 C, up-and-down and so on for 10-20 times.
That will produce halows from the center of the crystal and out.
You can see a nice on at my homepage, the page about crystal-glazes.
Take Care
Isak Isaksson
Velamsund
s-132 36 S-Boo
Sweden
08/7479721 (+4687479721)
isak=40mbox303.swipnet.se
http://home.swipnet.se/isaksson
| |
|