search  current discussion  categories  glazes - specific colors 

dark blue glaze

updated thu 6 may 99

 

Carole Steele on wed 5 may 99

I receive quite a few requests for this glaze and
will now post it for all.

Gilbert's Blue Glaze Cone 10 dark blue gloss
good on stoneware
similiar good results on soda/salt or reduction fire

Amounts are for a 333 gram test batch.

EPK Kaolin 42.0
Whiting 69.0
Flint 96.0
Custer Feldspar 102.0
Cobalt Carbonate 6.0
Red Iron Oxide 3.0
Titanium Dioxide 12.0
Bentonite 3.0

Carole in Louisiana
csteele=40centuryinter.net