search  current discussion  categories  glazes - crazing & crackle 

here's rhodes crackle slip recipe

updated tue 25 may 99

 

June Perry on mon 24 may 99

Someone requested this recently:

Rhodes White Crackle Slip cone 9-11

5 Borax
5 Zircopax
20 Custer Feldspar
15 Ball Clay
20 Calcined Kaolin
15 EPK
20 Flint

Regards,