^6 black glaze,native soil

updated tue 22 jun 99

 

Chris Schafale on mon 21 jun 99

Hi Katie,

Try Ron Roy's Cone 6 Black (referred to recently as "oo-la-la
black"). Very glossy, food safe, seems quite reliable, though
somewhat new. I've been told this is the best black folks have seen
for cone 6.

RR c6 black #2
-----------------
F4 SPAR................21.00
WHITING................6.00
TALC........................3.00
F3134....................26.00
EPK........................17.00
SILICA...................27.00
BENTONITE...........2.00
RED IRON OX........9.00
coblt carb.......... 1.00
----------
Total.....................112.00

Chris


> ----------------------------Original message----------------------------
> Hi! I'm looking for a stable Black cone 6 oxidation glaze. Preferably a
> glossy glaze. Its going to be used in a classroom setting so as reliable
> as possible.
> Pls e-mail me direct nativesoil@shimpoamerica.com
> Thanks-
> Katie
>
>