first of all, i'm sorry. i'm looking for "tan" color terra sigillata...like
mocha coffee. not "tin." if anyone have recipe of it, please tell me! : )
ok, now, i'll give you my recipes. all recipes are for cone 04.
Red
Ball Clay (OM-4) 200g
Water 1600g
Calgon 20g
Red Iron Oxide 200g
White
Ball Clay (OM-4) 400g
Water 1600g
Calgon 20g
Navy
Ball Clay (OM-4) 400g
Water 1600g
Calgon 10g
Manganese Diox. 20g
Cobalt Oxide 40g
Copper Oxide 20g
Green
Ball Clay (OM-4) 400g
Water 1600g
Calgon 20g
Add:
Chrome Oxide 20g
Light Yellow
Ball Clay (OM-4) 400g
Water 1600g
Calgon 20g
Add:
Vanadium
Pentaoxide 20g
Apache Red
Apach Clay 270g
Ball Clay (OM-4) 130g
Water 1600g
Calgon 20g
Pink
Ball Clay (OM-4) 200g
EPK 174g
Water 1600g
Calgon 20g
Yellow Iron Oxide 26g
read the second e-mail for more recipes.: )
| |
|