search  current discussion  categories  techniques - slips 

fw: porceilian slip?

updated mon 30 aug 99

 

ababy sharon on sun 29 aug 99

A question: Is this slip on greenware or bisque is it also Raku resist?
Thanks
Ababi
----- Original Message -----
From: Vince Pitelka
To:
Sent: Thursday, August 26, 1999 06:56
Subject: Re: porceilian slip?


> ----------------------------Original message----------------------------
> >Can anyone help me with a receipe for porcelain slip???
> >Any help will be greatly appreciated.
> >Bobbi Cats ( UTexas ceramics student)
>
> Bobbi -
> I am assuming you are looking for a decorating slip, > > All-Temperature
White Base Slip
> Kaolin ------------------- 34
> Ball Clay --------------- 20
> Potash Feldspar ---- 27
> Silica ------------------- 19
> Total ------------------- 100
> Plus: 8% Zircopax (opacifier)
>
> Good luck -
> - Vince
>
> Vince Pitelka - vpitelka@DeKalb.net
> Home 615/597-5376, work 615/597-6801 ext. 111, fax 615/597-6803
> Appalachian Center for Crafts
> Tennessee Technological University
> 1560 Craft Center Drive, Smithville TN 37166
>