Kimberly B. Severance on fri 10 sep 99
Hello Clayart Readers!
I must admit that I've been delinquent when it comes to reading the digest
regularly but I will skip the excuses. I've been in the studio
experiencing the learning curve first hand and am now in good shape except
for the glazing part of the process. Perhaps one of you knows of a nice
(STABLE!!!) Celadon glaze recipe for cone 05 that you could share. My
E-mail is Sevy@conknet.com. Your help would positively affect my
frustration level! Thank you! Kim Severance
irishjim@aol.com on mon 13 sep 99
irishji-@aol.com wrote:
original article:http://www.egroups.com/group/clayart/?start=52274
> ----------------------------Original message-------------------------
---
> Hello Clayart Readers!
> I must admit that I've been delinquent when it comes to
reading the digest
> regularly but I will skip the excuses. I've been in the studio
> experiencing the learning curve first hand and am now in good shape
except
> for the glazing part of the process. Perhaps one of you knows of a
nice
> (STABLE!!!) Celadon glaze recipe for cone 05 that you could share. My
> E-mail is Sevy@conknet.com. Your help would positively affect my
> frustration level! Thank you! Kim Severance
>
> I have an 08 glaze formula for a "Faux Celadon"that I personally have
never tried. You may want to test a small batch an see how it looks.
Percent Batch
Gerstley Borate 75% 375 Gram
EPK (Kaolin) 10% 50 "
Silica (200) 15% 75 "
Total 100% 500 "
add
Red Iron Oxide 2% 10 "
Good Luck
Irish jim
| |
|