arlene h. on fri 26 nov 99
are these glazes for cone 6 oxid~n? how can i tell? thanks for your
patience!
______________________________________________________
Get Your Private, Free Email at http://www.hotmail.com
Rudy Bauer on sun 28 nov 99
I have a good pink to burgandy for cone 6 oxidation I got from clayart.
It's reliable and beautiful from cones 5 to 7 which I've tried.
Gerstley borate 20.68
Nephsye 16.29
EPK 11.34
Whiting 19.52
Flint 32.16
Tin oxide 5.00
Green Chrome oxide 0.15
At 03:09 PM 11/26/99 -0500, you wrote:
>----------------------------Original message----------------------------
>are these glazes for cone 6 oxid~n? how can i tell? thanks for your
>patience!
>
>______________________________________________________
>Get Your Private, Free Email at http://www.hotmail.com
>
Chris Schafale on sun 28 nov 99
Yes. Sorry it wasn't clear. Burgundy Satin is actually better at
cone 5, as I think I said, but yes, it's ox. I think it would
probably run horribly in reduction, with all that iron acting as a
flux.
Chris
> ----------------------------Original message----------------------------
> are these glazes for cone 6 oxid~n? how can i tell? thanks for your
> patience!
>
> ______________________________________________________
> Get Your Private, Free Email at http://www.hotmail.com
>
>
Light One Candle Pottery
Fuquay-Varina, NC
candle@intrex.net
Rudy Bauer on mon 29 nov 99
Just had a full glaze load finish with spectacular results using this
glaze. Fired to cone 6.
At 10:51 AM 11/28/99 -0500, you wrote:
>----------------------------Original message----------------------------
>I have a good pink to burgandy for cone 6 oxidation I got from clayart.
>It's reliable and beautiful from cones 5 to 7 which I've tried.
>Gerstley borate 20.68
>Nephsye 16.29
>EPK 11.34
>Whiting 19.52
>Flint 32.16
>Tin oxide 5.00
>Green Chrome oxide 0.15
>
>At 03:09 PM 11/26/99 -0500, you wrote:
>>----------------------------Original message----------------------------
>>are these glazes for cone 6 oxid~n? how can i tell? thanks for your
>>patience!
>>
>>______________________________________________________
>>Get Your Private, Free Email at http://www.hotmail.com
>>
>
| |
|