Lorraine Pierce on fri 10 dec 99

Hi Sarah, your ^6 oxidation glaze is indeed a beauty, tho high in
manganese. Would you please post it to the list? My black and white
laser printer could not pick up the print from your web site, tho the
photos of the pot came thu very well.Thanks and good luck...(like the
name of your pottery!) Lori in New Port Richey Fl.

Nanci Bishof on sun 12 dec 99


In a message dated 12/10/99 2:41:08 PM, acody@ucsd.edu writes:

<< http://www.fortunecity.com/greenfield/runningbrook/455/grey.html >>
^6 ox Sarah's Shimmering Dusk
Gerstley Borate 20.4
Strontium Carb 9.6
Custer Feldspar 43
Silica 24.3
EPK 1
Whiting 1.6
Zircopax 15
Tin Ox 3
Copper Carb 3
Cobalt Carb 1.3
Manganese Diox 12

Lori,

I could barely make it out but was able to copy it line by line onto a reply
and then retype to get it in black & white format. Hope this helps. My
thoughts on the manganese too, but I don't do functional ware.

nanci

Sarah Lackey on sun 12 dec 99

as reuqested. . . :)

Sarah s Shimmering Grey Cone 6

Gerstly Borate 20.4 204 408
Strontium Carb 9.6 96 192
Custer 43 430 860
Silica 24.3 243 486
EPK 1 10 20
Whiting 1.6 16 32
Zircopax 10 100 200
Tin Oxide 3 30 60
Copper Carb 3 30 60
Cobalt Carb 1.5 15 30
Manganese Diox 12 120 240



>From: Lorraine Pierce
>Reply-To: Ceramic Arts Discussion List
>To: CLAYART@LSV.UKY.EDU
>Subject: Sarah's Shimmering Dusk Glaze
>Date: Fri, 10 Dec 1999 18:21:23 EST
>
>----------------------------Original message----------------------------
>Hi Sarah, your ^6 oxidation glaze is indeed a beauty, tho high in
>manganese. Would you please post it to the list? My black and white
>laser printer could not pick up the print from your web site, tho the
>photos of the pot came thu very well.Thanks and good luck...(like the
>name of your pottery!) Lori in New Port Richey Fl.

______________________________________________________
Get Your Private, Free Email at http://www.hotmail.com

Bobbi Bassett on mon 13 dec 99

In a message dated 12/10/99 6:22:13 PM Eastern Standard Time,
lorinfla@earthlink.net writes:

> My black and white
> laser printer could not pick up the print from your web site, tho the
> photos of the pot came thu very well.Thanks and good luck...(like the
> name of your pottery!) Lori in New Port Richey Fl.
>
Lori, If you highlight the text in the web site, then cut and paste it into
an email message box you can print it out just as if it was an email . That's
what I did and it worked fine on my old B&W HP printer. Good luck.

Bobbi in PA where it's cold and wet today