Opal Turtle Pottery
Glaze name: Kemp 17 (I call it Opalescent Wine Red)
Cone: 6 - 7 Oxidation or Reduction
Color: translucent red with purple streaks

Gerstley Borate 21.00 105.0 210
Neph Syenite 16.00 80.0 160
Kaolin 11.00 55.0 110
Whiting 20.00 100.0 200
Silica 32.00 160.0 320
Totals: 100.00 % 500.0 Gm

Also add:
Tin Oxide 5.00 25.0 50
Chrome Oxide 0.15 0.8 1.6




______________________________________________________
Get Your Private, Free Email at http://www.hotmail.com

Nancy Rogers on tue 14 dec 99

From: Sarah Lackey

It's a great translucent red with opalescent purple
streaks. . .You'll love it!

Sarah
Opal Turtle Pottery
Glaze name: Kemp 17 (I call it Opalescent Wine Red)
Cone: 6 - 7 Oxidation or Reduction
Color: translucent red with purple streaks

Gerstley Borate 21.00 105.0 210
Neph Syenite 16.00 80.0 160
Kaolin 11.00 55.0 110
Whiting 20.00 100.0 200
Silica 32.00 160.0 320
Totals: 100.00 % 500.0 Gm

Also add:
Tin Oxide 5.00 25.0 50
Chrome Oxide 0.15 0.8 1.6