search  current discussion  categories  glazes - misc 

new glaze

updated thu 23 dec 99

 

mel jacobson on wed 22 dec 99

does anyone know the source, or have you seen this glaze?
hi ho silver:
cone 10
yellow to orange, to silver.

thin application.

nephy sy 60
dolomite 18 (slight change from original)
ball clay 15
tin 4
bentonite 3

this is from st.paul potter mike norman.
he thinks it is a western u.s. glaze.

i am going to make some white slip
covering dark stoneware pots, and try it.
combo of white and dark....we will see.
really like some pots that i found of his, with
this glaze.
need a new millenium glaze.
mel/mn.
-10 f. this day.
but, as they say, no wind.

big moon coming round the bend.
http://www.pclink.com/melpots (website)
from minnetonka, minnesota, u.s.a.