Here=B4s some low-fire cr.-glazes:

Ferro 3110 45 gr
zinc oxide 25 gr
bentonite 3 gr., silica 19 gr
rutile 8 gr
+1220 deg. C/ If you have a slow kiln, adjust to +1210 de.C
--------
C-5/6 / Matt
Nephelinesyenite 52=25
Barium Carbonate /TOX 22=25
Whiting 19=25
Molybdenum oxide 3=25
Rutile 2=25
Litium carbonate 2=25
---------
C-06-04 / Matt
Silica 45=25
Litium carbonate 35=25
Kaolin 10=25
Soda ash 10=25
---------
The above=3Dcolour with diff. oxides
--------
C-07 / TRIPPLE-TOXIC
Red lead 80=25
Uranium oxide 15=25
Barium oxide 5=25
Wonderful red-orange.
-------
C-07/ DOUBLE-TOXIC
Red lead 80=25
Kaolin 14=25
Uranium-oxide 6
Orange-red galvan.
-----
C-011 Burnt red
Borax 57=25
Flint 28.6=25
RIO 14.4=25
-----
At my homepage, the end of =22glaze-page=22 you can see diff. mixes of =
oxides to
crystal-glazes.
Good Luck

All the best
Isak Isaksson
Velamsund
s-132 36 S-Boo
Sweden
08/7479721 (+4687479721)
isak=40mbox303.swipnet.se
http://home.swipnet.se/isaksson
Eller: welcome.to/isak

----- Ursprungligt meddelande -----
Fr=E5n: Jennifer Marchman =3Cjmarchman=40hotmail.com=3E
Till: =3CCLAYART=40LSV.UKY.EDU=3E
Skickat: den 8 februari 2000 20:03
=C4mne: low-fire crystalline glaze recipes


=3E ----------------------------Original message----------------------------
=3E I am looking for low-fire, Cone 06-04 crystalline glazes. All I have =
been
=3E able to find are high fire glazes. There is supposedly an article in
=3E December 1975's 'Ceramics Monthly' containing several cone 06 recipes. =
Does
=3E anyone have this article, or know of any other low-fire recipes?
=3E
=3E Thank you,
=3E Jennifer Marchman
=3E =
=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F==
5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5F=5=
F=5F=5F=5F
=3E Get Your Private, Free Email at http://www.hotmail.com
=3E