Deborah B. on mon 10 apr 00
Smart:
3134
Na20 10.3%
CaO 20.1%
B2O3 23.1%
SiO2 46.5 %
Moelcular Wght. 190.5
EPK
SiO2 45.91
Al2O3 38.71
Fe2O3 0.42
TiO2 0.34
CaO 0.09
MgO 0.12
K2O 0.22
Na2O 0.04
I.L. 14.16
Custer Feldspar
SiO2 68.5 Unit Molecular Formula Mol. Wght. 615
Al2O3 17.5
Fe2O3 0.08 K20 .69 Al2O3 1.05 SiO2 7.05
CaO 0.30 Na2O .31
MgO 0.01
K2O 10.4
Na2O 3.0
I.L. 0.3
Deborah
>From: Smart
>Reply-To: Ceramic Arts Discussion List
>To: CLAYART@LSV.UKY.EDU
>Subject: Need Chemical compositions by elements
>Date: Sun, 9 Apr 2000 21:05:43 EDT
>
>----------------------------Original message----------------------------
>------------------
>Hi,
>I have to make glazes calculations and I need to know exactly some
>informations
>about composition by elements (SiO2, Al2O3, K2O, Na2O, CaO,.... in %)
>
>Is someone able to give me the chemical composition of the following
>components
>:
>
>1) Frit 3134
>2) EPK
>3) Custer Feldspar
>
>Many thanks, Cordialement,
>Smart
______________________________________________________
Get Your Private, Free Email at http://www.hotmail.com
Lawrence Ewing on mon 10 apr 00
Hi,
You can get the composition of these materials and many others from the
following website:
MATRIX ADDITIONAL MATERIALS RESOURCE:
http://home.clear.net.nz/pages/Matrix2000/MatrialsWeb/default.htm
Lawrence Ewing
Senior Lecturer
Ceramics Department
School of Art
Otago Polytechnic
Dunedin
New Zealand
email: lewing@clear.net.nz
MATRIX GLAZE CALCULATION SOFTWARE:
http://home.clear.net.nz/pages/Matrix2000
GLAZETEACH:
http://home.clear.net.nz/pages/GlazeTeach
MATRIX TUTORIALS:
http://home.clear.net.nz/pages/lewing/MatrixTutorials
-----Original Message-----
From: Ceramic Arts Discussion List [mailto:CLAYART@LSV.UKY.EDU]On Behalf
Of Smart
Sent: Monday, April 10, 2000 1:06 PM
To: CLAYART@LSV.UKY.EDU
Subject: Need Chemical compositions by elements
----------------------------Original message----------------------------
------------------
Hi,
I have to make glazes calculations and I need to know exactly some
informations
about composition by elements (SiO2, Al2O3, K2O, Na2O, CaO,.... in %)
Is someone able to give me the chemical composition of the following
components
:
1) Frit 3134
2) EPK
3) Custer Feldspar
Many thanks, Cordialement,
Smart
Sharon31 on mon 10 apr 00
Hello Smart!
Here are 3 site in them, you can search for materials:
http://home.clear.net.nz/pages/Matrix2000/
http://art.sdsu.edu/ceramicsweb/
http://ceramicsearch.com/index.html
Good searching, Ababi
----- Original Message -----
From: Smart
To:
Sent: Monday, April 10, 2000 04:05
Subject: Need Chemical compositions by elements
----------------------------Original message----------------------------
------------------
Hi,
I have to make glazes calculations and I need to know exactly some
informations
about composition by elements (SiO2, Al2O3, K2O, Na2O, CaO,.... in %)
Is someone able to give me the chemical composition of the following
components
:
1) Frit 3134
2) EPK
3) Custer Feldspar
Many thanks, Cordialement,
Smart
Wade Blocker on mon 10 apr 00
----------
From: Smart
To: CLAYART@LSV.UKY.EDU
Subject: Need Chemical compositions by elements
Date: Sunday, April 09, 2000 7:05 PM
----------------------------Original message----------------------------
------------------
Hi,
I have to make glazes calculations and I need to know exactly some
informations
about composition by elements (SiO2, Al2O3, K2O, Na2O, CaO,.... in %)
Is someone able to give me the chemical composition of the following
components
:
1) Frit 3134
2) EPK
3) Custer Feldspar
Many thanks, Cordialement,
Smart
----------
Edgar Plastic Kaolin
sio2 al2o3 fe2o3 knao tio2 cao mgo Mol weight
2.040 1.000 .012 .016 .017 .008 .008 262.60
na2o cao b2o3 sio3
frit 3l34 10.2 20.1 23.2 46.5
Custer
na2o k2o al2o3 sio2 fe2o3 cao mgo ig.loss
3.0 10.4 l7.5 68.5 o.o8 0.30 trace 0.3
Hope this helps. Mia in ABQ
Smart on thu 13 apr 00
Dear Wade Blocker,
Many thanks for your help, I have to calculate some glazes properties and
these compositions was unknown for me. I am a new Clayarter since a week,
coming from France, and I try to help some american potters. So here the raw
materials are not the same compared to Europe.
You can visit my French web site on : http://perso.wanadoo.fr/smart2000/
May I ask you other formulas about raw materials ?
best regards,
Smart
----- Original Message -----
From: Wade Blocker
To:
Sent: Monday, April 10, 2000 10:31 PM
Subject: Re: Need Chemical compositions by elements
> ----------------------------Original message----------------------------
>
>
> ----------
> From: Smart
> To: CLAYART@LSV.UKY.EDU
> Subject: Need Chemical compositions by elements
> Date: Sunday, April 09, 2000 7:05 PM
>
> ----------------------------Original message----------------------------
> ------------------
> Hi,
> I have to make glazes calculations and I need to know exactly some
> informations
> about composition by elements (SiO2, Al2O3, K2O, Na2O, CaO,.... in %)
>
> Is someone able to give me the chemical composition of the following
> components
> :
>
> 1) Frit 3134
> 2) EPK
> 3) Custer Feldspar
>
> Many thanks, Cordialement,
> Smart
> ----------
>
>
> Edgar Plastic Kaolin
>
> sio2 al2o3 fe2o3 knao tio2 cao mgo Mol weight
> 2.040 1.000 .012 .016 .017 .008 .008 262.60
>
>
>
>
> na2o cao b2o3 sio3
> frit 3l34 10.2 20.1 23.2 46.5
>
>
>
>
>
> Custer
>
>
> na2o k2o al2o3 sio2 fe2o3 cao mgo ig.loss
> 3.0 10.4 l7.5 68.5 o.o8 0.30 trace 0.3
>
>
> Hope this helps. Mia in ABQ
David Hewitt on sat 15 apr 00
Hello Smart,
You may be interested in the raw material formulae that I have listed in
groups for comparison on my web site under 'Transporting Glaze Recipes'
http://www.dhpot.demon.co.uk
These lists were compiled largely to assist in taking US or UK recipes
and using local materials. I would be interested in knowing if French
pottery supplies differ much from UK supplies. Is such data available on
the internet, please?
David
In message , Smart writes
>----------------------------Original message----------------------------
>Dear Wade Blocker,
>Many thanks for your help, I have to calculate some glazes properties and
>these compositions was unknown for me. I am a new Clayarter since a week,
>coming from France, and I try to help some american potters. So here the raw
>materials are not the same compared to Europe.
>You can visit my French web site on : http://perso.wanadoo.fr/smart2000/
>May I ask you other formulas about raw materials ?
>
>best regards,
>Smart
>
>----- Original Message -----
>From: Wade Blocker
>To:
>Sent: Monday, April 10, 2000 10:31 PM
>Subject: Re: Need Chemical compositions by elements
>
>
>> ----------------------------Original message----------------------------
>>
>>
>> ----------
>> From: Smart
>> To: CLAYART@LSV.UKY.EDU
>> Subject: Need Chemical compositions by elements
>> Date: Sunday, April 09, 2000 7:05 PM
>>
>> ----------------------------Original message----------------------------
>> ------------------
>> Hi,
>> I have to make glazes calculations and I need to know exactly some
>> informations
>> about composition by elements (SiO2, Al2O3, K2O, Na2O, CaO,.... in %)
>>
>> Is someone able to give me the chemical composition of the following
>> components
>> :
>>
>> 1) Frit 3134
>> 2) EPK
>> 3) Custer Feldspar
>>
>> Many thanks, Cordialement,
>> Smart
>> ----------
>>
>>
>> Edgar Plastic Kaolin
>>
>> sio2 al2o3 fe2o3 knao tio2 cao mgo Mol weight
>> 2.040 1.000 .012 .016 .017 .008 .008 262.60
>>
>>
>>
>>
>> na2o cao b2o3 sio3
>> frit 3l34 10.2 20.1 23.2 46.5
>>
>>
>>
>>
>>
>> Custer
>>
>>
>> na2o k2o al2o3 sio2 fe2o3 cao mgo ig.loss
>> 3.0 10.4 l7.5 68.5 o.o8 0.30 trace 0.3
>>
>>
>> Hope this helps. Mia in ABQ
>
--
David Hewitt
David Hewitt Pottery ,
7 Fairfield Road, Caerleon, Newport,
South Wales, NP18 3DQ, UK. Tel:- +44 (0) 1633 420647
FAX:- +44 (0) 870 1617274
Web site http://www.dhpot.demon.co.uk
| |
|