search  current discussion  categories  glazes - cone 4-7 

marcia's msub ^6 reduction glazes (long)

updated sat 13 may 00

 

Marcia Selsor on wed 10 may 00

Dear Friends,
Here are our best glazes from the past 20 years and since being forced
to
drop chrome and Barium from our chemicals. We did substitute a chrome
Mason stain in a teal glaze.There are 14 with some bases listing
suggested colorants for variation. They look like stoneware to me. We
reduced at ^09-04 (about an hour) and again at ^6 tile the kilns even
out or for another hour. If trying for good coppers reds, keep the
atmosphere just slightly in reduction all the way. Lately I was throwing
wood sticks in as the kiln cooled for several hours after reaching
twmperature. My imagination or not, the reds looked great. -a clayart suggestion

Montana State University-Billings
^6 Our Best Reduction Shop glazes

1.Sexy Black (satin matt)

Whiting 11.75
Kona F4 Feldspar 54.5
EPK 6.5
Silics 25
Red Iron Oxide 10
Manganese Dioxide 2.5
110.25

Nice black matt glaze, does not run. Gold flecks develop in good reduction
Use caution with Manganese.

2. Marci's Matt

EPK 23
Dolomite 20
Neph. Syn. 38
Silica 18
Whiting 4
Gerstley Borate10
113

Lots of possibilities
a. Blue 1% Cobalt Carb
b. Light Green 1.5 % Nickel Carbonate
1.5% Red Iron Oxide
c. Light Blue .5% Cobalt Carbonate
2.5% Rutile
d.Gray Blue .5 Cobalt Carb
1.5 Nickel Carbonate
2.5 Rutile
e. Gray 2.5 Rutile
1.5 Nickel Carb.
f. Warm Tan 2.5 Rutile
2.5% Red Iron
"The surface is great for baking dishes. It is non-stick." Joyce Taylor Mayer

3. Clear (semi matt)
Whiting 18.5
Neph. Syn 25.8
EPK 18.8
Silica 31.1
Gerstley Borate 4.6

For nice celedon 1.5% Red Iron Oxide

4.Plum
Whiting 10
Silica 20
Custer Spar 30
Yellow Ochre 10

This can settle rock hard (add epson salts 2tbsp. per 10,000 grams) Good
Iron Red/plum

5. Ohata Red
Bone ash 14
Dolomite 8
Ger. Borate 4
Lithium Carb 4
Custer Spar 52
Kaolin 6
Silica 12

Add Red Iron Oxide 8
Great Tomato Iron red with gold flecks in the sun!
If thick it goes black.

6. Paul's Yellow
Frit 3134 45
Barium Frit 3247 20
Dolomite 10
EPKaolin 5
Zircopax 15
Whiting 3
Red Iron Oxide 3

Matt yellow very dry when thin

7. Turquoise
Neph Syn. 61.27
Strontium Carb 31.94
Silica 2.47
Copper Carb. 2.85
Lithium Carb. 14.7

May not be food safe. Nice smooth matt glaze.

8. Hammer Red Black
Custer Feld. 50
Ball Clay 10
Silica 10
Whiting 15
Iron Oxide 15

Thin is plum red, thick is black

9. Web Red (from Clayart
Neph. Syn 55.33
Gertsley Borate 12.61
Whiting 10.71
Silica 21.35

Add
copper carb .39
tin oxide .99

Oxblood use 1.5% tin
.4 copper carb
.4 Iron Oxide

11. Waxy White Liner (this base from a handout from Pullman, Wa. 1980)
Gerstley Borate 20
Neph Syen 30
EPK 13.3
Whiting 9.4
Talc 17.4
Silica 10
Zircopax 15
114.9
Good functional base glaze with these variations
Pumpkin (Oakleaf) 5% red iron oxide, 3% rutile
Gold 3% Rutile
Lavender 4% cobalt Carb (use sparingly)
Light Blue .5% cobalt carb and 3% rutile
Spicey Mustard 3% iron oxide plus 3% rutile

12. Nelson's Base (from the famous textbook recently heralded on the
book thread)
Custer Spar 64
Whiting 18
Ball Clay 9
Talc 5
96

Teal .75 Chrome (use Green Mason Stain 3%)
.25 Cobalt Carb.
Speckled Green .4% Cobalt Carb
2.5 Iron Oxide
Tan 3.5% Rutile
Blue 2.8 Cobalt Carb
Speckled Toad 8% Red Iron Oxide

13. F. Carlton Ball's Base
Custer Feldspar 36
Whiting 17.8
Cornwall Stone 17.8
Ball Clay 9
Rutile 12.9
Zinc 6.5
100
Speckled Green .25 Cobalt Carb plus 2.5 Iron Oxide

14.Linda's Moss Black (Actually a caramel turns bluer with age)
Kona F4 54
Whiting 14.7
Bentonite 2.4
Gerstley Borate 4
Neph Syen 6
Kaolin 2.66
Talc 3.5
Silica 11.6
Zircopax 2.0
102.86
Add
Red Iron Oxide 8
Rutile 6


--
Marcia Selsor
selsor@imt.net
http://www.imt.net/~mjbmls
http://www.imt.net/~mjbmls/spain99.html
http://www.silverhawk.com/ex99/selsor/welcome.html

eric nissen on thu 11 may 00

Marcia:
You're the BEST for sharing these glazes with us, Thank-you so much.
Sandra
Warm & sunny Woodstock, GA

Andi Cody on fri 12 may 00

I second that. Thanks for taking the time to post these glazes. We will
have a great time trying some of them out in our little gas kiln.

Andi in San Diego

At 05:39 PM 05/11/2000 EDT, you wrote:
>----------------------------Original message----------------------------
>Marcia:
>You're the BEST for sharing these glazes with us, Thank-you so much.
>Sandra
>Warm & sunny Woodstock, GA
>