search  current discussion  categories  glazes - cone 4-7 

fakeash cone 6

updated fri 12 may 00

 

Bob Bruch on thu 11 may 00

Someone had requested the formula for Tyler Fake Ash,
cone 5 to 6 Oxidation

Ferro Frit 3110 16
Red Art 48
GB 16
Dolomite 20

Total 100

Comment/Questions

1) I did one small test tile, very different results from thick to thin
applications, may break well on edges.

2) Would a replacement of a clay such as Newman for Red Art to obtain a
slight color variation work on a 1 to 1 replacement basis?